RAW MATERIALS | %, weight |
LAWS(71) | 34 gr |
WAX(68) | 2 gr |
WAX(69) | 1.3 gr |
Emulsifiers(70) | 1 gr |
Silicone Fluids 350 cSt(72) | 1.5 gr |
Silicone Fluids 10000 cSt(74) | 1.5 gr |
Rheology Modifiers(76) | 0.1 gr |
Water | 43.5 gr |
Calcined Kaolin(9) | 15 gr |
Preservative(77) | 0.1 gr |
Stir LAWS with low speed.
Add wax, emulsifiers, silicone fluids, and heat to 90°C until the wax dissolved.
Add rheology modifiers, mix for 20 minutes.
Add hot water (70°C) with high speed stirring add calcined kaolin mix for 20 minutes.
Stir slowly add preservative, mix for 30 minutes.